{"id":603,"date":"2018-10-17T00:14:55","date_gmt":"2018-10-16T16:14:55","guid":{"rendered":"https:\/\/plasticmoldco.com\/?p=603"},"modified":"2018-10-17T00:14:55","modified_gmt":"2018-10-16T16:14:55","slug":"chapter-25-1-residual-stress","status":"publish","type":"post","link":"https:\/\/www.plasticmoldco.com\/ko\/2018\/10\/17\/25\uc7a5-1-\uc794\ub958-\uc2a4\ud2b8\ub808\uc2a4\/","title":{"rendered":"25-1\uc7a5, \uc794\uc5ec \uc2a4\ud2b8\ub808\uc2a4"},"content":{"rendered":"<h1>\uc218\ucd95 \ubc0f \ub4a4\ud2c0\ub9bc \ubb38\uc81c\uc758 \uc8fc\ubc94<\/h1>\n<p>\uc794\ub958 \uc751\ub825\uc740 \uc131\ud615 \ubd80\ud488\uc5d0\uc11c \ubc1c\uc0dd\ud558\ub294 \uacf5\uc815 \uc720\ub3c4 \uc751\ub825\uc785\ub2c8\ub2e4. \uc720\ub3d9 \uc720\ub3c4\ud615 \ub610\ub294 \uc5f4 \uc720\ub3c4\ud615\uc77c \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc794\ub958 \uc751\ub825\uc740 \uc678\ubd80\uc5d0\uc11c \uac00\ud574\uc9c0\ub294 \uc751\ub825\uacfc \uc720\uc0ac\ud558\uac8c \ubd80\ud488\uc5d0 \uc601\ud5a5\uc744 \ubbf8\uce69\ub2c8\ub2e4. \ubd80\ud488\uc758 \uad6c\uc870\uc801 \ubb34\uacb0\uc131\uc744 \uadf9\ubcf5\ud560 \uc218 \uc788\uc744 \uc815\ub3c4\ub85c \uac15\ud558\uba74 \uc678\ubd80 \uc11c\ube44\uc2a4 \ud558\uc911\uc774 \uac00\ud574\uc9c0\uba74 \ubd80\ud488\uc774 \ubc30\ucd9c \uc2dc \ub4a4\ud2c0\ub9ac\uac70\ub098 \ub098\uc911\uc5d0 \uade0\uc5f4\uc774 \ubc1c\uc0dd\ud569\ub2c8\ub2e4. \uc794\ub958 \uc751\ub825\uc740 \ubd80\ud488 \uc218\ucd95\uacfc \ub4a4\ud2c0\ub9bc\uc758 \uc8fc\uc694 \uc6d0\uc778\uc785\ub2c8\ub2e4. \uce90\ube44\ud2f0 \ucda9\uc804 \uc911 \uc804\ub2e8 \uc751\ub825\uc744 \uc904\uc774\ub294 \uacf5\uc815 \uc870\uac74\uacfc \uc124\uacc4 \uc694\uc18c\ub294 \uc720\ub3d9\uc73c\ub85c \uc778\ud55c \uc794\ub958 \uc751\ub825\uc744 \uc904\uc774\ub294 \ub370 \ub3c4\uc6c0\uc774 \ub429\ub2c8\ub2e4. \ub9c8\ucc2c\uac00\uc9c0\ub85c \ucda9\ubd84\ud55c \ud328\ud0b9\uacfc \uade0\uc77c\ud55c \uae08\ud615 \ub0c9\uac01\uc744 \ucd09\uc9c4\ud558\ub294 \uacf5\uc815\uc740 \uc5f4\uc5d0 \uc758\ud55c \uc794\ub958 \uc751\ub825\uc744 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4. \uc12c\uc720\ub85c \ucc44\uc6cc\uc9c4 \uc7ac\ub8cc\uc758 \uacbd\uc6b0, \uade0\uc77c\ud55c \uae30\uacc4\uc801 \ud2b9\uc131\uc744 \ucd09\uc9c4\ud558\ub294 \uacf5\uc815 \uc870\uac74\uc774 \uc5f4\uc5d0 \uc758\ud55c \uc794\ub958 \uc751\ub825\uc744 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4.\u00a0<a title=\"\uc911\uad6d \uae08\ud615 \uacf5\uae09 \uc5c5\uccb4\" href=\"https:\/\/web.archive.org\/web\/20130131102842\/http:\/\/www.moldchina.org\/\" target=\"_blank\" rel=\"noopener\">\uc911\uad6d \uae08\ud615 \uacf5\uae09 \uc5c5\uccb4<\/a><\/p>\n<h1>\uc720\ub7c9\uc73c\ub85c \uc778\ud55c \uc794\ub958 \uc751\ub825<\/h1>\n<p>\uc751\ub825\uc744 \ubc1b\uc9c0 \uc54a\ub294 \uc7a5\uc1c4 \ud3f4\ub9ac\uba38 \ubd84\uc790\ub294 \uc6a9\uc735 \uc628\ub3c4\ubcf4\ub2e4 \ub192\uc740 \uc628\ub3c4(\uc989, \uc6a9\uc735 \uc0c1\ud0dc)\uc5d0\uc11c \ub79c\ub364 \ucf54\uc77c \ud3c9\ud615 \uc0c1\ud0dc\ub97c \ub530\ub974\ub294 \uacbd\ud5a5\uc774 \uc788\uc2b5\ub2c8\ub2e4. \ucc98\ub9ac\ud558\ub294 \ub3d9\uc548 \ud3f4\ub9ac\uba38\uac00 \uc804\ub2e8\ub418\uace0 \uae38\uc5b4\uc9c0\uba74\uc11c \ubd84\uc790\ub294 \ud750\ub984 \ubc29\ud5a5\uc73c\ub85c \ubc29\ud5a5\uc744 \uc7a1\uc2b5\ub2c8\ub2e4. \ud3f4\ub9ac\uba38 \ubd84\uc790\uac00 \ud3c9\ud615 \uc0c1\ud0dc\ub85c \uc644\uc804\ud788 \uc774\uc644\ub418\uae30 \uc804\uc5d0 \uc751\uace0\uac00 \ubc1c\uc0dd\ud558\uba74 \ubd84\uc790 \ubc30\ud5a5\uc774 \uace0\uc815\ub429\ub2c8\ub2e4.<br \/>\n\uc131\ud615 \ubd80\ud488. \uc774\ub7ec\ud55c \uc720\ud615\uc758 \ub3d9\uacb0 \uc751\ub825 \uc0c1\ud0dc\ub97c \ud754\ud788 \uc720\ub3d9 \uc720\ub3c4 \uc794\ub958 \uc751\ub825\uc774\ub77c\uace0 \ud569\ub2c8\ub2e4. \ud750\ub984 \ubc29\ud5a5\uc73c\ub85c \ub298\uc5b4\ub09c \ubd84\uc790 \ubc30\ud5a5\uc73c\ub85c \uc778\ud574 \ud750\ub984 \ubc29\ud5a5\uc5d0 \ud3c9\ud589\ud558\uace0 \uc218\uc9c1\uc778 \ubc29\ud5a5\uc73c\ub85c \uc774\ubc29\uc131, \ube44\uade0\uc77c \uc218\ucd95 \ubc0f \uae30\uacc4\uc801 \ud2b9\uc131\uc774 \ubc1c\uc0dd\ud569\ub2c8\ub2e4.<\/p>\n<h2>\uace0\uc815\ub41c \ubd84\uc790 \ubc29\ud5a5<\/h2>\n<p>\ub192\uc740 \uc804\ub2e8 \uc751\ub825\uacfc \uae08\ud615 \ubcbd\uc5d0 \uc778\uc811\ud55c \ub192\uc740 \ub0c9\uac01 \uc18d\ub3c4\uc758 \uc870\ud569\uc73c\ub85c \uc778\ud574 \ubd80\ud488 \ud45c\uba74 \ubc14\ub85c \uc544\ub798\uc5d0 \uace0\ub3c4\ub85c \ubc30\ud5a5\ub41c \uce35\uc774 \uc5bc\uc5b4\ubd99\uc2b5\ub2c8\ub2e4. \uc774\ub294 \uadf8\ub9bc 1\uc5d0 \uc124\uba85\ub418\uc5b4 \uc788\uc2b5\ub2c8\ub2e4. \uc774\ud6c4 \uc794\ub958 \uc720\ub3d9 \uc751\ub825\uc774 \ub192\uc740(\ub610\ub294 \ubc29\ud5a5\uc774 \uace0\uc815\ub41c) \ubd80\ud488\uc744 \uace0\uc628\uc5d0 \ub178\ucd9c\ud558\uba74 \uc751\ub825 \uc911 \uc77c\ubd80\uac00 \uc644\ud654\ub420 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \uc774\ub85c \uc778\ud574 \uc77c\ubc18\uc801\uc73c\ub85c \ubd80\ud488 \uc218\ucd95\uacfc \ub4a4\ud2c0\ub9bc\uc774 \ubc1c\uc0dd\ud569\ub2c8\ub2e4. \ub3d9\uacb0 \uce35\uc758 \ub2e8\uc5f4 \ud6a8\uacfc\ub85c \uc778\ud574 \uace0\uc628 \ucf54\uc5b4\uc758 \ud3f4\ub9ac\uba38 \uc6a9\uc735\uc774 \ub354 \ub192\uc740 \uc218\uc900\uc73c\ub85c \uc774\uc644\ub418\uc5b4 \uc800\ubd84\uc790 \ubc30\ud5a5 \uc601\uc5ed\uc73c\ub85c \uc774\uc5b4\uc9c8 \uc218 \uc788\uc2b5\ub2c8\ub2e4.\u00a0<a title=\"\uc911\uad6d \uae08\ud615 \uacf5\uae09 \uc5c5\uccb4\" href=\"https:\/\/web.archive.org\/web\/20130131102842\/http:\/\/www.moldchina.org\/\" target=\"_blank\" rel=\"noopener\">\uc911\uad6d \uae08\ud615 \uacf5\uae09 \uc5c5\uccb4<\/a><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-1303\" title=\"\ub0c9\ub3d9 \ubd84\uc790 \uc9c0\ud5a5\" src=\"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif\" alt=\"\ub0c9\ub3d9 \ubd84\uc790 \uc9c0\ud5a5\" width=\"579\" height=\"258\" \/><\/p>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\uadf8\ub9bc 1.<\/strong>\u00a0\ucda9\uc804 \ubc0f \ud3ec\uc7a5 \ub2e8\uacc4\uc5d0\uc11c \ubd84\uc790 \ubc30\ud5a5\uc774 \uace0\uc815\ub418\uc5b4 \uc794\ub958 \uc720\ub3d9 \uc751\ub825\uc774 \ubc1c\uc0dd\ud569\ub2c8\ub2e4.<br \/>\n(1) \ub192\uc740 \ub0c9\uac01, \uc804\ub2e8 \ubc0f \ubc30\ud5a5 \uc601\uc5ed (2) \ub0ae\uc740 \ub0c9\uac01, \uc804\ub2e8 \ubc0f \ubc30\ud5a5 \uc601\uc5ed<\/p>\n<h2>\uc720\ub7c9\uc73c\ub85c \uc778\ud55c \uc794\ub958 \uc2a4\ud2b8\ub808\uc2a4 \uac10\uc18c<\/h2>\n<p>\uc6a9\uc735\ubb3c\uc758 \uc804\ub2e8 \uc751\ub825\uc744 \uac10\uc18c\uc2dc\ud0a4\ub294 \uacf5\uc815 \uc870\uac74\uc740 \uc720\ub3d9 \uc720\ub3c4 \uc794\ub958 \uc751\ub825\uc758 \uc218\uc900\uc744 \uac10\uc18c\uc2dc\ud0b5\ub2c8\ub2e4. \uc77c\ubc18\uc801\uc73c\ub85c \uc720\ub3d9 \uc720\ub3c4 \uc794\ub958 \uc751\ub825\uc740 \uc5f4 \uc720\ub3c4 \uc794\ub958 \uc751\ub825\ubcf4\ub2e4 \ud55c \ubc30 \uc815\ub3c4 \uc791\uc2b5\ub2c8\ub2e4.\u00a0<a title=\"\uc911\uad6d \uae08\ud615 \uacf5\uae09 \uc5c5\uccb4\" href=\"https:\/\/web.archive.org\/web\/20130131102842\/http:\/\/www.moldchina.org\/\" target=\"_blank\" rel=\"noopener\">\uc911\uad6d \uae08\ud615 \uacf5\uae09 \uc5c5\uccb4<\/a><\/p>\n<ul>\n<li>\ub354 \ub192\uc740 \uc6a9\uc735 \uc628\ub3c4<\/li>\n<li>\ub354 \ub192\uc740 \uae08\ud615 \ubcbd \uc628\ub3c4<\/li>\n<li>\ub354 \uae34 \ucda9\uc804 \uc2dc\uac04(\ub354 \ub0ae\uc740 \uc6a9\uc735 \uc18d\ub3c4)<\/li>\n<li>\ud3ec\uc7a5 \uc555\ub825 \uac10\uc18c<\/li>\n<li>\ub354 \uc9e7\uc740 \ud750\ub984 \uacbd\ub85c.<\/li>\n<\/ul>\n<h1>\u00a0\uc5f4\ub85c \uc778\ud55c \uc794\ub958 \uc751\ub825<\/h1>\n<p>\uc5f4\ub85c \uc778\ud55c \uc794\ub958 \uc751\ub825\uc740 \ub2e4\uc74c\uacfc \uac19\uc740 \uc774\uc720\ub85c \ubc1c\uc0dd\ud569\ub2c8\ub2e4:<\/p>\n<ul>\n<li>\uacf5\uc815 \uc124\uc815\uc5d0\uc11c \uacf5\uc815 \uc644\ub8cc \uc2dc \ub3c4\ub2ec\ud55c \uc8fc\ubcc0 \uc870\uac74\uc73c\ub85c \uc628\ub3c4\uac00 \ub0b4\ub824\uac00\uba74 \uc7ac\ub8cc\uac00 \uc218\ucd95\ud569\ub2c8\ub2e4.<\/li>\n<li>\uc7ac\ub8cc\uac00 \uae08\ud615 \ubcbd\uc5d0\uc11c \uc911\uc559\uc73c\ub85c \uc751\uace0\ub420 \ub54c \uc7ac\ub8cc \uc694\uc18c\ub294 \uc11c\ub85c \ub2e4\ub978 \uc5f4-\uae30\uacc4\uc801 \uc774\ub825(\uc608: \ub0c9\uac01 \uc18d\ub3c4 \ubc0f \ud328\ud0b9 \uc555\ub825)\uc744 \uacbd\ud5d8\ud569\ub2c8\ub2e4.<\/li>\n<li>\uc555\ub825, \uc628\ub3c4, \ubd84\uc790 \ubc0f \uc12c\uc720 \ubc29\ud5a5\uc774 \ubc14\ub00c\uba74 \ubc00\ub3c4\uc640 \uae30\uacc4\uc801 \ud2b9\uc131\uc774 \ub2ec\ub77c\uc9d1\ub2c8\ub2e4.<\/li>\n<li>\ud2b9\uc815 \uae08\ud615 \uc81c\uc57d \uc870\uac74\uc740 \uc131\ud615\ub41c \ubd80\ud488\uc774 \ud3c9\uba74 \ubc29\ud5a5\uc73c\ub85c \uc218\ucd95\ud558\ub294 \uac83\uc744 \ubc29\uc9c0\ud569\ub2c8\ub2e4.<\/li>\n<\/ul>\n<h2>\ubb34\ub8cc \ub2f4\uae08\uc9c8 \uc608\uc2dc<\/h2>\n<p>\uc0ac\ucd9c \uc131\ud615 \uc911 \uc7ac\ub8cc \uc218\ucd95\uc740 \uade0\uc77c\ud55c \uc628\ub3c4\uc758 \uc77c\ubd80\uac00 \uac11\uc790\uae30 \ucc28\uac00\uc6b4 \uae08\ud615 \ubcbd\uc5d0 \ub07c\uc5b4\ub4dc\ub294 \uc790\uc720 \ub2f4\uae08\uc9c8 \uc608\uc2dc\ub97c \ud1b5\ud574 \ud3b8\ub9ac\ud558\uac8c \uc2dc\uc5f0\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4. \ucd08\uae30 \ub0c9\uac01 \ub2e8\uacc4\uc5d0\uc11c \uc678\ubd80 \ud45c\uba74\uce35\uc774 \ub0c9\uac01\ub418\uc5b4 \uc218\ucd95\ud558\uae30 \uc2dc\uc791\ud558\uba74 \ub728\uac70\uc6b4 \ucf54\uc5b4\uc758 \ud3f4\ub9ac\uba38 \ub300\ubd80\ubd84\uc740 \uc5ec\uc804\ud788 \uc6a9\uc735\ub418\uc5b4 \uc790\uc720\ub86d\uac8c \uc218\ucd95\ud569\ub2c8\ub2e4. \uadf8\ub7ec\ub098 \ub0b4\ubd80 \ucf54\uc5b4\uac00 \ub0c9\uac01\ub418\uba74 \uc774\ubbf8 \ub2e8\ub2e8\ud574\uc9c4 \uc678\ubd80 \uce35\uc5d0 \uc758\ud574 \uad6d\ubd80\uc801\uc778 \uc5f4 \uc218\ucd95\uc774 \uc81c\uc57d\uc744 \ubc1b\uc2b5\ub2c8\ub2e4. \uadf8 \uacb0\uacfc \uc544\ub798 \uadf8\ub9bc 2\uc640 \uac19\uc774 \ucf54\uc5b4\uc758 \uc7a5\ub825\uc774 \uc678\ubd80 \uce35\uc758 \uc555\ucd95\uacfc \uade0\ud615\uc744 \uc774\ub8e8\ub294 \uc77c\ubc18\uc801\uc778 \uc751\ub825 \ubd84\ud3ec \uc0c1\ud0dc\uac00 \ub429\ub2c8\ub2e4.<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-1304\" title=\"\ubb34\ub8cc \ub2f4\uae08\uc9c8 \uc608\uc81c\" src=\"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Free-quenching-example.gif\" alt=\"\ubb34\ub8cc \ub2f4\uae08\uc9c8 \uc608\uc81c\" width=\"579\" height=\"258\" \/><\/p>\n<p><strong>\uadf8\ub9bc 2.<\/strong>\u00a0\uc131\ud615 \ubd80\ud488 \uc804\uccb4\uc758 \ub0c9\uac01 \ubcc0\ud654\uc640 \uc628\ub3c4 \uc774\ub825\uc5d0 \ub300\ud55c \uc7ac\ub8cc\uc758 \ubc18\uc751\uc73c\ub85c \uc778\ud574 '\uc790\uc720 \ub2f4\uae08\uc9c8' \ubd80\ud488\uc5d0 \uc794\ub958 \uc5f4 \uc751\ub825\uc774 \ubc1c\uc0dd\ud569\ub2c8\ub2e4.<\/p>","protected":false},"excerpt":{"rendered":"<p>A culprit in shrinkage and warpage problems Residual stress is a process-induced stress, frozen in a molded part. It can be either\u00a0flow-induced or thermal-induced. Residual stresses affect a part similarly to externally applied stresses. If they are strong enough to overcome the structural integrity of the part, the part will warp upon ejection, or later [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_et_pb_use_builder":"","_et_pb_old_content":"","_et_gb_content_width":"","footnotes":""},"categories":[15],"tags":[],"class_list":["post-603","post","type-post","status-publish","format-standard","hentry","category-mould-technology-blog-1"],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v28.8 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker<\/title>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/www.plasticmoldco.com\/ko\/2018\/10\/17\/kapitel-25-1-restspanning\/\" \/>\n<meta property=\"og:locale\" content=\"ko_KR\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker\" \/>\n<meta property=\"og:description\" content=\"A culprit in shrinkage and warpage problems Residual stress is a process-induced stress, frozen in a molded part. It can be either\u00a0flow-induced or thermal-induced. Residual stresses affect a part similarly to externally applied stresses. If they are strong enough to overcome the structural integrity of the part, the part will warp upon ejection, or later [&hellip;]\" \/>\n<meta property=\"og:url\" content=\"https:\/\/www.plasticmoldco.com\/ko\/2018\/10\/17\/kapitel-25-1-restspanning\/\" \/>\n<meta property=\"og:site_name\" content=\"Plastic Mold | China Mold Maker\" \/>\n<meta property=\"article:published_time\" content=\"2018-10-16T16:14:55+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif\" \/>\n<meta name=\"author\" content=\"admin\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\uae00\uc4f4\uc774\" \/>\n\t<meta name=\"twitter:data1\" content=\"admin\" \/>\n\t<meta name=\"twitter:label2\" content=\"\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04\" \/>\n\t<meta name=\"twitter:data2\" content=\"3\ubd84\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"Article\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\"},\"author\":{\"name\":\"admin\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/person\\\/8377d429cf711f79d68feec3e8648777\"},\"headline\":\"Chapter 25-1, Residual stress\",\"datePublished\":\"2018-10-16T16:14:55+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\"},\"wordCount\":657,\"commentCount\":0,\"publisher\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\",\"articleSection\":[\"Mould Technology Blog 1\"],\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"CommentAction\",\"name\":\"Comment\",\"target\":[\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#respond\"]}]},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\",\"name\":\"Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\",\"datePublished\":\"2018-10-16T16:14:55+00:00\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#breadcrumb\"},\"inLanguage\":\"ko-KR\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\",\"url\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\",\"contentUrl\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/www.plasticmoldco.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Chapter 25-1, Residual stress\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#website\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/\",\"name\":\"Plastic Mold | China Mold Maker\",\"description\":\"Are you looking for injection mold china? We are plastic mold maker\",\"publisher\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ko-KR\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#organization\",\"name\":\"Plastic Mold | China Mold Maker\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/uploads\\\/2018\\\/10\\\/nlogon.png\",\"contentUrl\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/uploads\\\/2018\\\/10\\\/nlogon.png\",\"width\":204,\"height\":54,\"caption\":\"Plastic Mold | China Mold Maker\"},\"image\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/logo\\\/image\\\/\"}},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/person\\\/8377d429cf711f79d68feec3e8648777\",\"name\":\"admin\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ko-KR\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/litespeed\\\/avatar\\\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/litespeed\\\/avatar\\\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842\",\"contentUrl\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/litespeed\\\/avatar\\\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842\",\"caption\":\"admin\"},\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/ko\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"25-1\uc7a5, \uc794\ub958 \uc751\ub825 - \ud50c\ub77c\uc2a4\ud2f1 \uae08\ud615 | \uc911\uad6d \uae08\ud615 \uc81c\uc870\uc5c5\uccb4","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/www.plasticmoldco.com\/ko\/2018\/10\/17\/kapitel-25-1-restspanning\/","og_locale":"ko_KR","og_type":"article","og_title":"Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker","og_description":"A culprit in shrinkage and warpage problems Residual stress is a process-induced stress, frozen in a molded part. It can be either\u00a0flow-induced or thermal-induced. Residual stresses affect a part similarly to externally applied stresses. If they are strong enough to overcome the structural integrity of the part, the part will warp upon ejection, or later [&hellip;]","og_url":"https:\/\/www.plasticmoldco.com\/ko\/2018\/10\/17\/kapitel-25-1-restspanning\/","og_site_name":"Plastic Mold | China Mold Maker","article_published_time":"2018-10-16T16:14:55+00:00","og_image":[{"url":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","type":"","width":"","height":""}],"author":"admin","twitter_card":"summary_large_image","twitter_misc":{"\uae00\uc4f4\uc774":"admin","\uc608\uc0c1 \ub418\ub294 \ud310\ub3c5 \uc2dc\uac04":"3\ubd84"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"Article","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#article","isPartOf":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/"},"author":{"name":"admin","@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/person\/8377d429cf711f79d68feec3e8648777"},"headline":"Chapter 25-1, Residual stress","datePublished":"2018-10-16T16:14:55+00:00","mainEntityOfPage":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/"},"wordCount":657,"commentCount":0,"publisher":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#organization"},"image":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage"},"thumbnailUrl":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","articleSection":["Mould Technology Blog 1"],"inLanguage":"ko-KR","potentialAction":[{"@type":"CommentAction","name":"Comment","target":["https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#respond"]}]},{"@type":"WebPage","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/","url":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/","name":"25-1\uc7a5, \uc794\ub958 \uc751\ub825 - \ud50c\ub77c\uc2a4\ud2f1 \uae08\ud615 | \uc911\uad6d \uae08\ud615 \uc81c\uc870\uc5c5\uccb4","isPartOf":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#website"},"primaryImageOfPage":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage"},"image":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage"},"thumbnailUrl":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","datePublished":"2018-10-16T16:14:55+00:00","breadcrumb":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#breadcrumb"},"inLanguage":"ko-KR","potentialAction":[{"@type":"ReadAction","target":["https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/"]}]},{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage","url":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","contentUrl":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif"},{"@type":"BreadcrumbList","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/www.plasticmoldco.com\/"},{"@type":"ListItem","position":2,"name":"Chapter 25-1, Residual stress"}]},{"@type":"WebSite","@id":"https:\/\/www.plasticmoldco.com\/el\/#website","url":"https:\/\/www.plasticmoldco.com\/el\/","name":"\ud50c\ub77c\uc2a4\ud2f1 \uae08\ud615 | \uc911\uad6d \uae08\ud615 \uc81c\uc870\uc5c5\uccb4","description":"\uc0ac\ucd9c \uae08\ud615 \uc911\uad6d\uc744 \ucc3e\uace0 \uacc4\uc2ed\ub2c8\uae4c? \uc6b0\ub9ac\ub294 \ud50c\ub77c\uc2a4\ud2f1 \uae08\ud615 \uc81c\uc870\uc5c5\uccb4\uc785\ub2c8\ub2e4.","publisher":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/www.plasticmoldco.com\/el\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ko-KR"},{"@type":"Organization","@id":"https:\/\/www.plasticmoldco.com\/el\/#organization","name":"\ud50c\ub77c\uc2a4\ud2f1 \uae08\ud615 | \uc911\uad6d \uae08\ud615 \uc81c\uc870\uc5c5\uccb4","url":"https:\/\/www.plasticmoldco.com\/el\/","logo":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/logo\/image\/","url":"https:\/\/www.plasticmoldco.com\/wp-content\/uploads\/2018\/10\/nlogon.png","contentUrl":"https:\/\/www.plasticmoldco.com\/wp-content\/uploads\/2018\/10\/nlogon.png","width":204,"height":54,"caption":"Plastic Mold | China Mold Maker"},"image":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/logo\/image\/"}},{"@type":"Person","@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/person\/8377d429cf711f79d68feec3e8648777","name":"\uad00\ub9ac\uc790","image":{"@type":"ImageObject","inLanguage":"ko-KR","@id":"https:\/\/www.plasticmoldco.com\/wp-content\/litespeed\/avatar\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842","url":"https:\/\/www.plasticmoldco.com\/wp-content\/litespeed\/avatar\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842","contentUrl":"https:\/\/www.plasticmoldco.com\/wp-content\/litespeed\/avatar\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842","caption":"admin"},"url":"https:\/\/www.plasticmoldco.com\/ko\/author\/admin\/"}]}},"_links":{"self":[{"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/posts\/603","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/comments?post=603"}],"version-history":[{"count":0,"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/posts\/603\/revisions"}],"wp:attachment":[{"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/media?parent=603"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/categories?post=603"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ko\/wp-json\/wp\/v2\/tags?post=603"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}