{"id":603,"date":"2018-10-17T00:14:55","date_gmt":"2018-10-16T16:14:55","guid":{"rendered":"https:\/\/plasticmoldco.com\/?p=603"},"modified":"2018-10-17T00:14:55","modified_gmt":"2018-10-16T16:14:55","slug":"chapter-25-1-residual-stress","status":"publish","type":"post","link":"https:\/\/www.plasticmoldco.com\/ja\/2018\/10\/17\/\u7b2c25\u7ae0-1-\u6b8b\u7559\u5fdc\u529b\/","title":{"rendered":"\u7b2c25-1\u7ae0\u6b8b\u7559\u5fdc\u529b"},"content":{"rendered":"<h1>\u53ce\u7e2e\u3068\u53cd\u308a\u306e\u554f\u984c\u306e\u539f\u56e0<\/h1>\n<p>\u6b8b\u7559\u5fdc\u529b\u3068\u306f\u3001\u6210\u5f62\u54c1\u306b\u51cd\u7d50\u3057\u3066\u3044\u308b\u52a0\u5de5\u8a98\u8d77\u5fdc\u529b\u306e\u3053\u3068\u3067\u3059\u3002\u6b8b\u7559\u5fdc\u529b\u306b\u306f\u6d41\u52d5\u8a98\u8d77\u306e\u3082\u306e\u3068\u71b1\u8a98\u8d77\u306e\u3082\u306e\u304c\u3042\u308a\u307e\u3059\u3002\u6b8b\u7559\u5fdc\u529b\u306f\u3001\u5916\u90e8\u304b\u3089\u52a0\u3048\u3089\u308c\u308b\u5fdc\u529b\u3068\u540c\u69d8\u306b\u90e8\u54c1\u306b\u5f71\u97ff\u3092\u4e0e\u3048\u307e\u3059\u3002\u6b8b\u7559\u5fdc\u529b\u304c\u90e8\u54c1\u306e\u69cb\u9020\u7684\u5b8c\u5168\u6027\u306b\u6253\u3061\u52dd\u3064\u307b\u3069\u5f37\u3044\u5834\u5408\u3001\u5916\u90e8\u304b\u3089\u306e\u4f7f\u7528\u8377\u91cd\u304c\u52a0\u308f\u308b\u3068\u3001\u90e8\u54c1\u306f\u5c04\u51fa\u6642\u306b\u53cd\u3063\u305f\u308a\u3001\u5f8c\u306b\u5272\u308c\u305f\u308a\u3057\u307e\u3059\u3002\u6b8b\u7559\u5fdc\u529b\u306f\u3001\u90e8\u54c1\u306e\u53ce\u7e2e\u3068\u53cd\u308a\u306e\u4e3b\u306a\u539f\u56e0\u3067\u3059\u3002\u30ad\u30e3\u30d3\u30c6\u30a3\u5145\u586b\u6642\u306e\u305b\u3093\u65ad\u5fdc\u529b\u3092\u4f4e\u6e1b\u3059\u308b\u30d7\u30ed\u30bb\u30b9\u6761\u4ef6\u3084\u8a2d\u8a08\u8981\u7d20\u306f\u3001\u6d41\u52d5\u306b\u8d77\u56e0\u3059\u308b\u6b8b\u7559\u5fdc\u529b\u306e\u4f4e\u6e1b\u306b\u5f79\u7acb\u3061\u307e\u3059\u3002\u540c\u69d8\u306b\u3001\u5341\u5206\u306a\u5145\u586b\u3068\u5747\u4e00\u306a\u91d1\u578b\u51b7\u5374\u3092\u4fc3\u9032\u3059\u308b\u5de5\u7a0b\u6761\u4ef6\u306f\u3001\u71b1\u306b\u3088\u308b\u6b8b\u7559\u5fdc\u529b\u3092\u4f4e\u6e1b\u3057\u307e\u3059\u3002\u7e4a\u7dad\u5145\u586b\u6750\u6599\u306e\u5834\u5408\u3001\u5747\u4e00\u306a\u6a5f\u68b0\u7684\u7279\u6027\u3092\u4fc3\u9032\u3059\u308b\u5de5\u7a0b\u6761\u4ef6\u306f\u3001\u71b1\u306b\u3088\u308b\u6b8b\u7559\u5fdc\u529b\u3092\u4f4e\u6e1b\u3057\u307e\u3059\u3002\u00a0<a title=\"\u4e2d\u56fd\u91d1\u578b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc\" href=\"https:\/\/web.archive.org\/web\/20130131102842\/http:\/\/www.moldchina.org\/\" target=\"_blank\" rel=\"noopener\">\u4e2d\u56fd\u91d1\u578b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc<\/a><\/p>\n<h1>\u6d41\u52d5\u8a98\u8d77\u6b8b\u7559\u5fdc\u529b<\/h1>\n<p>\u5fdc\u529b\u306e\u304b\u304b\u3063\u3066\u3044\u306a\u3044\u9577\u9396\u30dd\u30ea\u30de\u30fc\u5206\u5b50\u306f\u3001\u6eb6\u878d\u6e29\u5ea6\u3088\u308a\u9ad8\u3044\u6e29\u5ea6\uff08\u3059\u306a\u308f\u3061\u6eb6\u878d\u72b6\u614b\uff09\u3067\u306f\u3001\u5e73\u8861\u306e\u30e9\u30f3\u30c0\u30e0\u30b3\u30a4\u30eb\u72b6\u614b\u306b\u306a\u308b\u50be\u5411\u304c\u3042\u308b\u3002\u52a0\u5de5\u4e2d\u3001\u30dd\u30ea\u30de\u30fc\u306f\u526a\u65ad\u3055\u308c\u3066\u4f38\u9577\u3059\u308b\u305f\u3081\u3001\u5206\u5b50\u306f\u6d41\u308c\u65b9\u5411\u306b\u914d\u5411\u3059\u308b\u3002\u30dd\u30ea\u30de\u30fc\u5206\u5b50\u304c\u5e73\u8861\u72b6\u614b\u307e\u3067\u5b8c\u5168\u306b\u5f1b\u7de9\u3059\u308b\u524d\u306b\u51dd\u56fa\u304c\u8d77\u3053\u308b\u3068\u3001\u5206\u5b50\u914d\u5411\u306f\u30dd\u30ea\u30de\u30fc\u5206\u5b50\u5185\u306b\u56fa\u5b9a\u3055\u308c\u308b\u3002<br \/>\n\u6210\u5f62\u90e8\u54c1\u3002\u3053\u306e\u7a2e\u306e\u51cd\u7d50\u5fdc\u529b\u72b6\u614b\u306f\u3001\u3057\u3070\u3057\u3070\u6d41\u52d5\u8a98\u8d77\u6b8b\u7559\u5fdc\u529b\u3068\u547c\u3070\u308c\u307e\u3059\u3002\u6d41\u52d5\u65b9\u5411\u306b\u5206\u5b50\u914d\u5411\u304c\u5f15\u304d\u4f38\u3070\u3055\u308c\u308b\u305f\u3081\u3001\u6d41\u52d5\u65b9\u5411\u306b\u5e73\u884c\u306a\u65b9\u5411\u3068\u5782\u76f4\u306a\u65b9\u5411\u3067\u53ce\u7e2e\u7387\u3084\u6a5f\u68b0\u7684\u6027\u8cea\u306b\u7570\u65b9\u6027\u3001\u4e0d\u5747\u4e00\u6027\u304c\u751f\u3058\u307e\u3059\u3002<\/p>\n<h2>\u51cd\u308a\u3064\u3044\u305f\u5206\u5b50\u914d\u5411<\/h2>\n<p>\u9ad8\u3044\u305b\u3093\u65ad\u5fdc\u529b\u3068\u91d1\u578b\u58c1\u306b\u96a3\u63a5\u3059\u308b\u9ad8\u3044\u51b7\u5374\u901f\u5ea6\u306e\u7d44\u307f\u5408\u308f\u305b\u306b\u3088\u308a\u3001\u90e8\u54c1\u8868\u9762\u306e\u76f4\u4e0b\u306b\u51cd\u7d50\u3057\u305f\u9ad8\u914d\u5411\u5c64\u304c\u5b58\u5728\u3059\u308b\u3002\u3053\u308c\u3092\u56f31\u306b\u793a\u3059\u3002\u9ad8\u6b8b\u7559\u6d41\u52d5\u5fdc\u529b\uff08\u307e\u305f\u306f\u51cd\u7d50\u3057\u305f\u914d\u5411\uff09\u3092\u6709\u3059\u308b\u90e8\u54c1\u306f\u3001\u305d\u306e\u5f8c\u9ad8\u6e29\u306b\u66dd\u3055\u308c\u308b\u3053\u3068\u306b\u3088\u308a\u3001\u5fdc\u529b\u306e\u4e00\u90e8\u304c\u7de9\u548c\u3055\u308c\u308b\u53ef\u80fd\u6027\u304c\u3042\u308a\u307e\u3059\u3002\u305d\u306e\u7d50\u679c\u3001\u90e8\u54c1\u306e\u53ce\u7e2e\u3084\u53cd\u308a\u304c\u751f\u3058\u308b\u306e\u304c\u4e00\u822c\u7684\u3067\u3059\u3002\u51cd\u7d50\u5c64\u306e\u65ad\u71b1\u52b9\u679c\u306b\u3088\u308a\u3001\u30db\u30c3\u30c8\u30b3\u30a2\u5185\u306e\u30dd\u30ea\u30de\u30fc\u6eb6\u878d\u7269\u306f\u3088\u308a\u9ad8\u5ea6\u306b\u7de9\u548c\u3059\u308b\u3053\u3068\u304c\u3067\u304d\u3001\u4f4e\u5206\u5b50\u914d\u5411\u9818\u57df\u304c\u5f62\u6210\u3055\u308c\u308b\u3002\u00a0<a title=\"\u4e2d\u56fd\u91d1\u578b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc\" href=\"https:\/\/web.archive.org\/web\/20130131102842\/http:\/\/www.moldchina.org\/\" target=\"_blank\" rel=\"noopener\">\u4e2d\u56fd\u91d1\u578b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc<\/a><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-1303\" title=\"\u51cd\u7d50\u5206\u5b50\u30aa\u30ea\u30a8\u30f3\u30bf\" src=\"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif\" alt=\"\u51cd\u7d50\u5206\u5b50\u30aa\u30ea\u30a8\u30f3\u30bf\" width=\"579\" height=\"258\" \/><\/p>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u56f31.<\/strong>\u00a0\u5145\u586b\u30fb\u5305\u88c5\u6bb5\u968e\u3067\u306e\u5206\u5b50\u914d\u5411\u306e\u51cd\u7d50\u306b\u3088\u308b\u6b8b\u7559\u6d41\u52d5\u5fdc\u529b\u306e\u767a\u751f\u3002<br \/>\n(1) \u9ad8\u51b7\u5374\u3001\u305b\u3093\u65ad\u3001\u914d\u5411\u30be\u30fc\u30f3 (2) \u4f4e\u51b7\u5374\u3001\u305b\u3093\u65ad\u3001\u914d\u5411\u30be\u30fc\u30f3<\/p>\n<h2>\u30d5\u30ed\u30fc\u306b\u3088\u308b\u6b8b\u7559\u5fdc\u529b\u306e\u4f4e\u6e1b<\/h2>\n<p>\u6eb6\u878d\u7269\u306e\u305b\u3093\u65ad\u5fdc\u529b\u3092\u4f4e\u6e1b\u3059\u308b\u30d7\u30ed\u30bb\u30b9\u6761\u4ef6\u306f\u3001\u6d41\u52d5\u8a98\u8d77\u6b8b\u7559\u5fdc\u529b\u306e\u30ec\u30d9\u30eb\u3092\u4f4e\u6e1b\u3059\u308b\u3002\u4e00\u822c\u306b\u3001\u6d41\u52d5\u8a98\u8d77\u6b8b\u7559\u5fdc\u529b\u306f\u71b1\u8a98\u8d77\u6b8b\u7559\u5fdc\u529b\u3088\u308a\u30821\u6841\u5c0f\u3055\u3044\u3002\u00a0<a title=\"\u4e2d\u56fd\u91d1\u578b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc\" href=\"https:\/\/web.archive.org\/web\/20130131102842\/http:\/\/www.moldchina.org\/\" target=\"_blank\" rel=\"noopener\">\u4e2d\u56fd\u91d1\u578b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc<\/a><\/p>\n<ul>\n<li>\u3088\u308a\u9ad8\u3044\u6eb6\u878d\u6e29\u5ea6<\/li>\n<li>\u91d1\u578b\u58c1\u6e29\u5ea6\u306e\u4e0a\u6607<\/li>\n<li>\u5145\u586b\u6642\u9593\u304c\u9577\u3044\uff08\u6eb6\u878d\u901f\u5ea6\u304c\u4f4e\u3044\uff09<\/li>\n<li>\u30d1\u30c3\u30ad\u30f3\u30b0\u5727\u306e\u4f4e\u4e0b<\/li>\n<li>\u3088\u308a\u77ed\u3044\u6d41\u8def\u3002<\/li>\n<\/ul>\n<h1>\u00a0\u71b1\u306b\u3088\u308b\u6b8b\u7559\u5fdc\u529b<\/h1>\n<p>\u71b1\u306b\u3088\u308b\u6b8b\u7559\u5fdc\u529b\u306f\u6b21\u306e\u3088\u3046\u306a\u7406\u7531\u3067\u767a\u751f\u3059\u308b\uff1a<\/p>\n<ul>\n<li>\u30d7\u30ed\u30bb\u30b9\u8a2d\u5b9a\u6e29\u5ea6\u304b\u3089\u30d7\u30ed\u30bb\u30b9\u5b8c\u4e86\u6642\u306b\u5230\u9054\u3059\u308b\u5468\u56f2\u6761\u4ef6\u307e\u3067\u6e29\u5ea6\u304c\u4e0b\u304c\u308b\u3068\u3001\u6750\u6599\u306f\u53ce\u7e2e\u3059\u308b\u3002<\/li>\n<li>\u6750\u6599\u304c\u92f3\u578b\u306e\u58c1\u304b\u3089\u4e2d\u5fc3\u306b\u5411\u304b\u3063\u3066\u51dd\u56fa\u3059\u308b\u969b\u3001\u6750\u6599\u8981\u7d20\u306f\u7570\u306a\u308b\u71b1\u6a5f\u68b0\u5c65\u6b74\uff08\u4f8b\u3048\u3070\u3001\u7570\u306a\u308b\u51b7\u5374\u901f\u5ea6\u3084\u5145\u586b\u5727\u529b\uff09\u3092\u7d4c\u9a13\u3059\u308b\u3002<\/li>\n<li>\u5727\u529b\u3001\u6e29\u5ea6\u3001\u5206\u5b50\u3084\u7e4a\u7dad\u306e\u914d\u5411\u304c\u5909\u5316\u3059\u308b\u3068\u3001\u5bc6\u5ea6\u3084\u6a5f\u68b0\u7684\u7279\u6027\u304c\u5909\u5316\u3059\u308b\u3002<\/li>\n<li>\u7279\u5b9a\u306e\u91d1\u578b\u5236\u7d04\u306b\u3088\u308a\u3001\u6210\u5f62\u54c1\u306f\u5e73\u9762\u65b9\u5411\u306b\u53ce\u7e2e\u3057\u306a\u3044\u3002<\/li>\n<\/ul>\n<h2>\u30d5\u30ea\u30fc\u30af\u30a8\u30f3\u30c1\u306e\u4f8b<\/h2>\n<p>\u5c04\u51fa\u6210\u5f62\u4e2d\u306e\u6750\u6599\u306e\u53ce\u7e2e\u306f\u3001\u6e29\u5ea6\u304c\u5747\u4e00\u306a\u90e8\u54c1\u304c\u7a81\u7136\u51b7\u305f\u3044\u91d1\u578b\u58c1\u3067\u631f\u307e\u308c\u308b\u30d5\u30ea\u30fc\u30af\u30a8\u30f3\u30c1\u306e\u4f8b\u3067\u7c21\u4fbf\u306b\u793a\u3059\u3053\u3068\u304c\u3067\u304d\u308b\u3002\u5916\u5074\u306e\u8868\u9762\u5c64\u304c\u51b7\u3048\u3066\u53ce\u7e2e\u3057\u59cb\u3081\u308b\u521d\u671f\u306e\u51b7\u5374\u6bb5\u968e\u3067\u306f\u3001\u9ad8\u6e29\u306e\u30b3\u30a2\u306e\u30dd\u30ea\u30de\u30fc\u306e\u5927\u90e8\u5206\u306f\u307e\u3060\u6eb6\u3051\u3066\u304a\u308a\u3001\u81ea\u7531\u306b\u53ce\u7e2e\u3059\u308b\u3053\u3068\u304c\u3067\u304d\u307e\u3059\u3002\u3057\u304b\u3057\u3001\u5185\u90e8\u30b3\u30a2\u304c\u51b7\u3048\u308b\u306b\u3064\u308c\u3066\u3001\u5c40\u6240\u7684\u306a\u71b1\u53ce\u7e2e\u306f\u3059\u3067\u306b\u786c\u3044\u5916\u90e8\u5c64\u306b\u3088\u3063\u3066\u62d8\u675f\u3055\u308c\u308b\u3002\u305d\u306e\u7d50\u679c\u3001\u4e0b\u306e\u56f32\u306b\u793a\u3059\u3088\u3046\u306b\u3001\u30b3\u30a2\u306e\u5f35\u529b\u3068\u5916\u5c64\u306e\u5727\u7e2e\u304c\u91e3\u308a\u5408\u3063\u305f\u5178\u578b\u7684\u306a\u5fdc\u529b\u5206\u5e03\u72b6\u614b\u306b\u306a\u308b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-1304\" title=\"\u30d5\u30ea\u30fc\u30af\u30a8\u30f3\u30c1\u30f3\u30b0\u306e\u4f8b\" src=\"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Free-quenching-example.gif\" alt=\"\u30d5\u30ea\u30fc\u30af\u30a8\u30f3\u30c1\u30f3\u30b0\u306e\u4f8b\" width=\"579\" height=\"258\" \/><\/p>\n<p><strong>\u56f32.<\/strong>\u00a0\u6210\u5f62\u54c1\u5168\u4f53\u306e\u51b7\u5374\u306e\u3070\u3089\u3064\u304d\u3068\u3001\u6e29\u5ea6\u5c65\u6b74\u306b\u5bfe\u3059\u308b\u6750\u6599\u306e\u53cd\u5fdc\u306b\u8d77\u56e0\u3059\u308b\u3001\u300c\u81ea\u7531\u713c\u5165\u308c\u300d\u90e8\u54c1\u306e\u6b8b\u7559\u71b1\u5fdc\u529b\u306e\u767a\u751f\u3002<\/p>","protected":false},"excerpt":{"rendered":"<p>A culprit in shrinkage and warpage problems Residual stress is a process-induced stress, frozen in a molded part. It can be either\u00a0flow-induced or thermal-induced. Residual stresses affect a part similarly to externally applied stresses. If they are strong enough to overcome the structural integrity of the part, the part will warp upon ejection, or later crack, when external service load is applied. Residual stresses are the main cause of part shrinkage and warpage. The process conditions and design elements that reduce shear stress during cavity filling will help to reduce flow-induced residual stress. Likewise, those that promote sufficient packing and uniform mold cooling will reduce thermal-induced residual stress. For fiber-filled [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_et_pb_use_builder":"","_et_pb_old_content":"","_et_gb_content_width":"","footnotes":""},"categories":[15],"tags":[],"class_list":["post-603","post","type-post","status-publish","format-standard","hentry","category-mould-technology-blog-1"],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v28.8 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker<\/title>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/www.plasticmoldco.com\/ja\/2018\/10\/17\/kapitel-25-1-restspanning\/\" \/>\n<meta property=\"og:locale\" content=\"ja_JP\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker\" \/>\n<meta property=\"og:description\" content=\"A culprit in shrinkage and warpage problems Residual stress is a process-induced stress, frozen in a molded part. It can be either\u00a0flow-induced or thermal-induced. Residual stresses affect a part similarly to externally applied stresses. If they are strong enough to overcome the structural integrity of the part, the part will warp upon ejection, or later crack, when external service load is applied. Residual stresses are the main cause of part shrinkage and warpage. The process conditions and design elements that reduce shear stress during cavity filling will help to reduce flow-induced residual stress. Likewise, those that promote sufficient packing and uniform mold cooling will reduce thermal-induced residual stress. For fiber-filled [&hellip;]\" \/>\n<meta property=\"og:url\" content=\"https:\/\/www.plasticmoldco.com\/ja\/2018\/10\/17\/kapitel-25-1-restspanning\/\" \/>\n<meta property=\"og:site_name\" content=\"Plastic Mold | China Mold Maker\" \/>\n<meta property=\"article:published_time\" content=\"2018-10-16T16:14:55+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif\" \/>\n<meta name=\"author\" content=\"admin\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"\u57f7\u7b46\u8005\" \/>\n\t<meta name=\"twitter:data1\" content=\"admin\" \/>\n\t<meta name=\"twitter:label2\" content=\"\u63a8\u5b9a\u8aad\u307f\u53d6\u308a\u6642\u9593\" \/>\n\t<meta name=\"twitter:data2\" content=\"3\u5206\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"Article\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\"},\"author\":{\"name\":\"admin\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/person\\\/8377d429cf711f79d68feec3e8648777\"},\"headline\":\"Chapter 25-1, Residual stress\",\"datePublished\":\"2018-10-16T16:14:55+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\"},\"wordCount\":657,\"commentCount\":0,\"publisher\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#organization\"},\"image\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\",\"articleSection\":[\"Mould Technology Blog 1\"],\"inLanguage\":\"ja\",\"potentialAction\":[{\"@type\":\"CommentAction\",\"name\":\"Comment\",\"target\":[\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#respond\"]}]},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\",\"name\":\"Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#website\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\"},\"image\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\"},\"thumbnailUrl\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\",\"datePublished\":\"2018-10-16T16:14:55+00:00\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#breadcrumb\"},\"inLanguage\":\"ja\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/\"]}]},{\"@type\":\"ImageObject\",\"inLanguage\":\"ja\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#primaryimage\",\"url\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\",\"contentUrl\":\"https:\\\/\\\/web.archive.org\\\/web\\\/20130131102842im_\\\/http:\\\/\\\/www.moldchina.org\\\/wp-content\\\/uploads\\\/2011\\\/10\\\/Frozen-in-molecular-orienta.gif\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/sv\\\/2018\\\/10\\\/17\\\/kapitel-25-1-restspanning\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/www.plasticmoldco.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Chapter 25-1, Residual stress\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#website\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/\",\"name\":\"Plastic Mold | China Mold Maker\",\"description\":\"Are you looking for injection mold china? We are plastic mold maker\",\"publisher\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"ja\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#organization\",\"name\":\"Plastic Mold | China Mold Maker\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ja\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/uploads\\\/2018\\\/10\\\/nlogon.png\",\"contentUrl\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/uploads\\\/2018\\\/10\\\/nlogon.png\",\"width\":204,\"height\":54,\"caption\":\"Plastic Mold | China Mold Maker\"},\"image\":{\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/logo\\\/image\\\/\"}},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/el\\\/#\\\/schema\\\/person\\\/8377d429cf711f79d68feec3e8648777\",\"name\":\"admin\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"ja\",\"@id\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/litespeed\\\/avatar\\\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842\",\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/litespeed\\\/avatar\\\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842\",\"contentUrl\":\"https:\\\/\\\/www.plasticmoldco.com\\\/wp-content\\\/litespeed\\\/avatar\\\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842\",\"caption\":\"admin\"},\"url\":\"https:\\\/\\\/www.plasticmoldco.com\\\/ja\\\/author\\\/admin\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"\u7b2c25-1\u7ae0 \u6b8b\u7559\u5fdc\u529b-\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u91d1\u578b\uff5c\u4e2d\u56fd\u91d1\u578b\u30e1\u30fc\u30ab\u30fc","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/www.plasticmoldco.com\/ja\/2018\/10\/17\/kapitel-25-1-restspanning\/","og_locale":"ja_JP","og_type":"article","og_title":"Chapter 25-1, Residual stress - Plastic Mold | China Mold Maker","og_description":"A culprit in shrinkage and warpage problems Residual stress is a process-induced stress, frozen in a molded part. It can be either\u00a0flow-induced or thermal-induced. Residual stresses affect a part similarly to externally applied stresses. If they are strong enough to overcome the structural integrity of the part, the part will warp upon ejection, or later crack, when external service load is applied. Residual stresses are the main cause of part shrinkage and warpage. The process conditions and design elements that reduce shear stress during cavity filling will help to reduce flow-induced residual stress. Likewise, those that promote sufficient packing and uniform mold cooling will reduce thermal-induced residual stress. For fiber-filled [&hellip;]","og_url":"https:\/\/www.plasticmoldco.com\/ja\/2018\/10\/17\/kapitel-25-1-restspanning\/","og_site_name":"Plastic Mold | China Mold Maker","article_published_time":"2018-10-16T16:14:55+00:00","og_image":[{"url":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","type":"","width":"","height":""}],"author":"admin","twitter_card":"summary_large_image","twitter_misc":{"\u57f7\u7b46\u8005":"admin","\u63a8\u5b9a\u8aad\u307f\u53d6\u308a\u6642\u9593":"3\u5206"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"Article","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#article","isPartOf":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/"},"author":{"name":"admin","@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/person\/8377d429cf711f79d68feec3e8648777"},"headline":"Chapter 25-1, Residual stress","datePublished":"2018-10-16T16:14:55+00:00","mainEntityOfPage":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/"},"wordCount":657,"commentCount":0,"publisher":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#organization"},"image":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage"},"thumbnailUrl":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","articleSection":["Mould Technology Blog 1"],"inLanguage":"ja","potentialAction":[{"@type":"CommentAction","name":"Comment","target":["https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#respond"]}]},{"@type":"WebPage","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/","url":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/","name":"\u7b2c25-1\u7ae0 \u6b8b\u7559\u5fdc\u529b-\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u91d1\u578b\uff5c\u4e2d\u56fd\u91d1\u578b\u30e1\u30fc\u30ab\u30fc","isPartOf":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#website"},"primaryImageOfPage":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage"},"image":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage"},"thumbnailUrl":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","datePublished":"2018-10-16T16:14:55+00:00","breadcrumb":{"@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#breadcrumb"},"inLanguage":"ja","potentialAction":[{"@type":"ReadAction","target":["https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/"]}]},{"@type":"ImageObject","inLanguage":"ja","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#primaryimage","url":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif","contentUrl":"https:\/\/web.archive.org\/web\/20130131102842im_\/http:\/\/www.moldchina.org\/wp-content\/uploads\/2011\/10\/Frozen-in-molecular-orienta.gif"},{"@type":"BreadcrumbList","@id":"https:\/\/www.plasticmoldco.com\/sv\/2018\/10\/17\/kapitel-25-1-restspanning\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/www.plasticmoldco.com\/"},{"@type":"ListItem","position":2,"name":"Chapter 25-1, Residual stress"}]},{"@type":"WebSite","@id":"https:\/\/www.plasticmoldco.com\/el\/#website","url":"https:\/\/www.plasticmoldco.com\/el\/","name":"\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u91d1\u578b\uff5c\u4e2d\u56fd\u91d1\u578b\u30e1\u30fc\u30ab\u30fc","description":"\u3042\u306a\u305f\u306f\u5c04\u51fa\u6210\u5f62\u91d1\u578b\u4e2d\u56fd\u3092\u63a2\u3057\u3066\u3044\u307e\u3059\u304b\uff1f\u79c1\u9054\u306f\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u578b\u30e1\u30fc\u30ab\u30fc\u3067\u3059","publisher":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/www.plasticmoldco.com\/el\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"ja"},{"@type":"Organization","@id":"https:\/\/www.plasticmoldco.com\/el\/#organization","name":"\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u91d1\u578b\uff5c\u4e2d\u56fd\u91d1\u578b\u30e1\u30fc\u30ab\u30fc","url":"https:\/\/www.plasticmoldco.com\/el\/","logo":{"@type":"ImageObject","inLanguage":"ja","@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/logo\/image\/","url":"https:\/\/www.plasticmoldco.com\/wp-content\/uploads\/2018\/10\/nlogon.png","contentUrl":"https:\/\/www.plasticmoldco.com\/wp-content\/uploads\/2018\/10\/nlogon.png","width":204,"height":54,"caption":"Plastic Mold | China Mold Maker"},"image":{"@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/logo\/image\/"}},{"@type":"Person","@id":"https:\/\/www.plasticmoldco.com\/el\/#\/schema\/person\/8377d429cf711f79d68feec3e8648777","name":"\u7ba1\u7406\u8005","image":{"@type":"ImageObject","inLanguage":"ja","@id":"https:\/\/www.plasticmoldco.com\/wp-content\/litespeed\/avatar\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842","url":"https:\/\/www.plasticmoldco.com\/wp-content\/litespeed\/avatar\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842","contentUrl":"https:\/\/www.plasticmoldco.com\/wp-content\/litespeed\/avatar\/dc9e67dc3cb4dac8041577aae375cd6d.jpg?ver=1794110842","caption":"admin"},"url":"https:\/\/www.plasticmoldco.com\/ja\/author\/admin\/"}]}},"_links":{"self":[{"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/posts\/603","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/comments?post=603"}],"version-history":[{"count":0,"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/posts\/603\/revisions"}],"wp:attachment":[{"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/media?parent=603"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/categories?post=603"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.plasticmoldco.com\/ja\/wp-json\/wp\/v2\/tags?post=603"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}